Characteristics of the material 27KH2N2M1F ( 27H2N2M1F, 27Õ2Í2Ì1Ô ).
Material :
27KH2N2M1F ( 27H2N2M1F, 27Õ2Í2Ì1Ô )
Classification :
Die tool steel
Chemical composition in % of the material 27KH2N2M1F ( 27H2N2M1F, 27Õ2Í2Ì1Ô ) .
C
Si
Mn
Ni
S
P
Cr
Mo
V
0.25 - 0.3
0.17 - 0.37
0.5 - 0.8
1.4 - 1.8
max 0.03
max 0.03
2 - 2.5
0.8 - 1
0.2 - 0.3
Mechanical properties under Ò=20oÑ of the material 27KH2N2M1F ( 27H2N2M1F, 27Õ2Í2Ì1Ô ) .
Assortment
Dimension
Direct.
sâ
sT
d5
y
KCU
Heat treatment
-
mm
-
MPa
MPa
%
%
kJ / m2
-
Forging
to 700
1300
1200
9
Normalizing and drawing
Technological properties of the material 27KH2N2M1F ( 27H2N2M1F, 27Õ2Í2Ì1Ô ) .
Weldability:
hard weldability.
Flakes :
weakly predisposed
Temper brittleness:
weakly predisposed
Specification :
Mechanical properties :
sâ
- Tensile strength , [MPa]
sT
- Yield stress, [MPa]
d5
- Specific elongation at fracture , [ % ]
y
- Reduction of area , [ % ]
KCU
- Impact strength , [ kJ / m2]
HB
- Brinell hardness , [MPa]
Weldability :
without limitations
- welding is done without heating and subsequent heat treeting
limited weldability
- welding is possible under heating up to 100-120 grade and subsequent heat treeting
hard weldability
- obtaining the quality welding needs the additional operations:heating up to 200-300 grade; the heat treeting ia annealing
Database of steels and alloys (Marochnik) contains information about chemical composition and properties of 1500 steels and alloys (stainless steel, alloy steel, carbone steel, structural steel, tool steel, cast iron, aluminum alloy, titanium alloy, copper alloy, nickel alloy, magnesium alloy and others). Helpfull for specialists in material technology, structural engineer, mechanical engineer, metallurgy and metal trader